The short answer
Remove everything that is not clean base metal from the weld area (oil, grease, rust, paint, mill scale and coatings), then make sure the joint fits together properly. Contaminants can cause porosity (gas holes), weak fusion, spatter and unstable arcs, and some produce hazardous fumes. How much prep is needed depends on the metal and process, but clean bare metal is a good default.
Step-by-step preparation
- Degrease first. Wipe off oil, grease and cutting fluid with a suitable solvent or degreaser before grinding, so you don’t smear and grind contaminants into the surface. Let solvents fully evaporate.
- Remove coatings and scale. Grind or sand off rust, paint and mill scale (the dark, flaky layer on hot-rolled steel) in and around the joint. Many guides suggest clearing at least about an inch on each side, and more for thicker work or high-quality requirements. An angle grinder with a flap disc or grinding wheel does most of the work, and a wire brush handles lighter surface rust.
- Do a final wipe. After grinding, remove dust and residue from the bare metal, especially for TIG or other high-quality work.
- Prepare the ground. Grind a clean spot for the work clamp. A poor ground connection causes erratic arcs and wasted time.
- Cut and bevel as needed. Thicker material is often beveled so the weld can reach the full depth. Remove burrs and sharp edges left from cutting.
- Fit up and clamp. Align the parts with consistent gaps. Clamps, magnets, jigs and fixtures or tack welds hold them in place. Poor fit-up is a common cause of distortion and burn-through.
Preparing specific metals
- Mild and carbon steel: Grind off mill scale and rust to bright metal. This is the most forgiving case.
- Stainless steel: Use abrasives and brushes reserved for stainless. Tools used on carbon steel can leave iron particles that contaminate the surface and affect corrosion resistance.
- Aluminum: The oxide layer melts at a much higher temperature than the metal beneath, so it must be removed just before welding, typically with a dedicated stainless brush or suitable abrasive, then wiped down. Avoid contaminating the surface with oil from gloved hands or dirty tools.
- Galvanized steel: Grind the zinc coating off the weld zone. Zinc fume can make you ill (often called metal fume fever), so use good ventilation and, where appropriate, respiratory protection.
- Cast iron: Often oil-soaked and brittle; see welding cast iron for crack-stopping and groove prep.
Differences by process
- TIG needs the cleanest surface and clean filler rod, because it has little tolerance for contamination.
- MIG also needs clean metal, but is more forgiving of light surface variation than TIG.
- Stick and self-shielded flux-cored tolerate some rust and scale better, though cleaner metal still gives better results. See TIG vs MIG and flux-cored vs MIG.
- Resistance processes depend on a consistent, conductive surface; coatings and scale can affect current flow. See resistance spot welding.
Joint design and fit-up
The joint type affects prep. A butt joint on thick plate typically needs a bevel and root gap; a lap or tee joint usually needs clean overlapping faces. See the five basic weld joints for the options.
Safety notes
- Never weld near chlorinated solvents or their vapors, such as some brake and parts cleaners. Heat and UV light can break them down into toxic gases. Clean parts and let the area air out first.
- Be cautious with unknown coatings and plating. Cadmium, for example, is hazardous and should not be welded without proper controls.
- Wear eye protection, gloves and hearing protection while grinding, and keep flammable materials away from sparks.
- Check the safety data sheets for the cleaners and coatings you work with.
A broader equipment checklist is in welding processes and equipment.