Why fit-up matters
Fit-up is how the two pipe ends are prepared, aligned, spaced and tacked before welding. A well-fitted joint makes the root pass easier and reduces defects. A poor one causes burn-through, lack of penetration, slag traps and misalignment that is hard to fix after the fact. Many experienced welders say a good share of a weld’s quality is decided at the fit-up stage.
The dimensions in this article are typical examples. For real work, take them from your welding procedure specification (WPS), drawing or test instructions.
Prepare the pipe ends
- Cut square. Pipe ends should be cut square so the gap is even all the way around.
- Bevel. Cut or grind the bevel, either with a bevel machine, a plasma or oxy-fuel cutter followed by grinding, or a hand grinder. Machine beveling gives the most consistent results.
- Clean. Remove mill scale, rust, paint, oil and moisture from the bevel and a short distance (often around an inch) back from it on the inside and outside. Clean to bright metal where required. On stainless and alloys, use clean dedicated tools.
- Deburr. Take burrs off the inside edge of the pipe, so they do not interfere with fit-up or trap slag.
Bevel angle and root face
Most pipe butt joints use a V-groove. Two numbers define it:
- Bevel angle. A common bevel on pipe is around 30 to 37.5 degrees per side, giving an included angle of 60 to 75 degrees. A 37.5 degree bevel is a standard in piping codes for many butt joints. Wider angles use more filler and add distortion, and narrower angles make the groove harder to reach.
- Root face (land). The root face is the flat, unbeveled area at the bottom of the bevel, commonly about 1/16 inch (roughly 1.5 mm) or slightly more. Some TIG setups use a very small or zero land, and some stick root techniques use a land of about 1/8 inch. A land helps resist burn-through, and a land that is too heavy can make full penetration difficult.
If you need to compare how a land changes the root pass with different electrodes, see can you use 7018 for a root pass?
Setting the root gap
The root gap is the space between the two pipe ends at the bottom of the groove. It is a balance:
- Too tight, and the arc cannot get through to fuse the root, leaving incomplete penetration.
- Too wide, and the puddle can fall through or become difficult to bridge, which leads to burn-through, a concave root or excess weld metal inside.
Typical gaps for open-root pipe are in the range of about 1/16 to 1/8 inch (roughly 1.5 to 3 mm), with the best number depending on the process, electrode or wire size, and root face. Stick roots with a cellulosic electrode often use a gap near the upper end of that range, and TIG roots with filler rod and a smaller land may use a smaller gap. Your procedure may show something different.
A simple way to set a gap is to use a spacer such as a welding rod or a small piece of wire of the right diameter, or purpose-made gap tools or pipe clamps. Check the gap at several points around the joint.
Alignment and high-low
Both pipe ends should line up on the inside so the inner surfaces meet. A step between the two inside surfaces is called high-low (or “hi-lo”). Codes and procedures limit how much is acceptable; see visual weld inspection for how it is checked. Excessive high-low makes the root pass harder to run, since one side of the joint receives less heat than the other and the weld has to climb a step.
Tips:
- Use pipe clamps, alignment fixtures or V-blocks to hold pipes in line.
- Rotate the pipes slightly to find the best match when wall thickness or ovality varies.
- Check alignment with a straightedge or angle iron along the outside of the pipe, and also by feel or sight on the inside.
- For fittings and flanges, check that the flange faces are square and bolt holes are aligned as the drawing requires.
Tack welds
Tack welds hold the fit-up together until the root pass is done.
- Number and placement. Four tacks at 12, 3, 6 and 9 o’clock are common on small to medium pipe. Larger pipe may need more, depending on the procedure. Some welders use three tacks equally spaced.
- Size. Keep them small, a short bead about the size the procedure allows, and made with the same process and filler type that the root pass will use if required by the WPS.
- Feather the ends. Grind or file the ends of each tack so they taper down. A tack with a smooth, thin start and end is easier to tie into without a lump or a stop-start defect. “Feathering” is frequently mentioned for test coupons.
- Quality. Tacks must be sound. Cracked or porous tacks can break or end up inside the final weld. Remove bad ones and redo them.
- Position. If the joint will be welded in a fixed position, place tacks where they will be easiest to tie into, and avoid putting heavy tacks at the bottom of the pipe, where overhead welding is hardest. See pipe welding positions.
Common fit-up mistakes
- Uneven gap, wide on one side and tight on the other
- Bevels cut at different angles on each pipe
- Heavy or lumpy tacks that are not feathered
- Leaving mill scale or oil on the joint
- Misalignment and high-low that is more than the procedure allows
- Moving the pipe after tacking, so the gap closes up or opens
- Tacks that are too few for the pipe size, so the joint pulls in as it cools
Check before you weld
A short checklist before the root pass:
- Is the joint clean and burr-free?
- Is the bevel and root face as the WPS or drawing requires?
- Is the gap even and within the allowed range at every tack?
- Is the inside alignment within the allowed high-low?
- Are the tacks sound and feathered?
- Is the pipe supported so it will not shift or sag?
Once the fit-up is right, move on to the root, hot, fill and cap passes. If you are preparing coupons for a qualification, see the 6G pipe welding test.