Stick Welding

How to Lay a Weld Bead

Learn how to lay a stick weld bead: preparing the plate, stringer and weave beads, reading the puddle, ending a bead without a crater, and fixing common problems.

On this page
  1. What is a weld bead?
  2. Prepare the plate and machine
  3. Laying a stringer bead step by step
  4. Weave beads
  5. Reading the puddle and bead
  6. Ending (terminating) a bead
  7. Restarting and overlapping beads
  8. Cleaning and inspecting
  9. Troubleshooting bead problems

What is a weld bead?

A weld bead is the strip of solidified metal left behind when you make a pass along a joint. Laying a bead means running the arc along the work so that the molten pool fuses with the base metal and the filler, and then freezes into a regular ridge. Practising beads on flat plate is the standard way to learn stick welding, because every other weld you make is built from them.

Prepare the plate and machine

Laying a stringer bead step by step

A stringer bead is a straight bead with little or no side-to-side movement. It is where most people should start.

  1. Strike the arc at the start point using a scratch or tap start (see arc welding lessons).
  2. Establish the puddle. Pause briefly so a molten pool forms and the arc settles.
  3. Set the angle. Lean the rod a small amount in the direction of travel and keep it square to the plate from the side. Travel direction is discussed in do you push or pull when arc welding.
  4. Move steadily. Travel at a speed that keeps the puddle a consistent width, feeding the rod down as it burns to maintain arc length.
  5. Watch the puddle and slag. The slag should trail behind the puddle, not run ahead of it.
  6. Finish by filling the crater (below).

Weave beads

Once stringers are consistent, you can practise a weave to make a wider bead. Move the rod side to side with a small, even motion, pausing briefly at each edge so the metal fills in against the plate rather than leaving undercut. As a general guide, keep weave width modest (many instructors suggest not much more than two to three times the rod diameter for stick welding), and use stringers instead for narrow gaps or when heat input must be limited. The trade-offs are covered in stringer beads vs weaving.

Reading the puddle and bead

Experienced welders learn to judge the weld from the puddle while they are making it, and from the finished bead afterwards. A good bead typically has:

  • evenly spaced ripples,
  • a consistent width and height,
  • smooth tie-in at the edges, with no deep grooves or sharp overlaps,
  • no visible holes or surface porosity.

Ending (terminating) a bead

If you simply lift the rod at the end of a pass, the arc leaves a depression called a crater, which can crack (see crater and star cracks). When preparing to finish a bead:

  • Slow your travel slightly or pause for a moment at the end to let the crater fill.
  • Reduce the arc length by a small amount, or make a brief circular motion to fill the crater, then lift away.
  • Do not stab the rod or snap the arc away abruptly.

Restarting and overlapping beads

To continue a bead after a rod runs out, chip the slag from the crater, then strike the arc slightly ahead of the crater, move back into it, and then proceed. This lets the new metal tie into the old crater. When making adjacent beads, overlap each by roughly a third to a half of the previous bead width, and clean the slag between passes.

Cleaning and inspecting

Allow the weld to cool slightly, then chip the slag with a chipping hammer and brush with a wire brush. Wear eye protection when chipping, since slag can fly. Examine the bead for cracks, pinholes, undercut and overlap. Visual weld inspection explains what to look for. If you are practising, keep your plates and compare them over time.

Troubleshooting bead problems

  • Narrow, tall, ropey bead: often too fast or the current too low.
  • Wide, flat bead with a lot of spatter: current may be too high or the arc too long.
  • Undercut at the edges: amperage too high, arc too long, or the rod angle off. See undercut causes, limits and fixes.
  • Slag trapped in the weld: travelling too slowly so slag rolls ahead, or poor cleaning between passes.
  • Pinholes or porosity: damp rods, dirty metal or too long an arc.
  • Rod freezing: see why your stick electrode keeps sticking.

When a bead goes wrong, change one thing at a time, so you can tell which adjustment fixed it.

The complete guide to stick welding

How Arc Welding Works: Stick, MMA and the Welding Arc
Read the guide

Keep exploring

Guides from other topics

All topics →