Weld Inspection and Defects

Undercut in Welding: Causes, Limits and Fixes

Undercut is a groove melted into the base metal beside a weld. Learn what causes it, how to avoid it in your technique, how it's judged, and how to repair it.

On this page
  1. What undercut is
  2. Why undercut matters
  3. Common causes
  4. How to avoid it
  5. How undercut is inspected and measured
  6. Acceptable limits
  7. Repairing undercut

What undercut is

Undercut is a groove or notch melted into the base metal along the toe of a weld (the edge where the weld meets the plate) that has not been filled in by weld metal. It can occur on the face of a weld, or at the root. In a fillet weld it commonly appears along the upper toe on the vertical plate, where the arc melts the plate and the metal sags rather than flowing back into the gap.

It is one of the most common visual defects, and one of the easiest to spot with a flashlight at a low angle.

Why undercut matters

The base metal at the toe is thinner than it should be, so the cross-section is reduced. More importantly, the notch acts as a stress concentrator. Under cyclic or fatigue loading, cracks can start from the sharp edge of an undercut. That is why codes tend to limit undercut more strictly for structures under fatigue or dynamic loading, and for critical pressure piping.

Shallow, smooth undercut in a statically loaded part may be of limited concern, but the acceptance decision belongs to the governing code, not to rules of thumb.

Common causes

Undercut generally happens when the arc melts more base metal at the edge than the filler metal can replace. Typical reasons:

  • Excessive current or voltage. Too much heat melts the edge of the joint faster than it is filled.
  • Travel speed too fast. The pool doesn’t have time to fill the melted edge.
  • Arc too long. A long arc spreads heat and digs the edges.
  • Wrong electrode or torch angle. Pointing the arc too much at one plate, especially the vertical member of a fillet, melts that plate without enough filler.
  • Poor weaving technique. Moving across the joint too fast or not pausing at the edges leaves grooves where the metal isn’t filled.
  • Oversized electrode or wire for the joint, or too high a wire feed rate in MIG.
  • Poor shielding gas selection for the process, in some cases. Certain gas mixes give wider, flatter beads than others.
  • Magnetic arc blow that deflects the arc toward one edge.
  • Welding position. Vertical and overhead positions make it harder for metal to fill the edge.

How to avoid it

  • Lower the current or voltage a little if you are getting a groove at the edges, within the range allowed by the procedure.
  • Slow down slightly, so the puddle has time to fill to the edge.
  • Shorten the arc and keep it consistent.
  • Aim the arc correctly. For a fillet weld, direct the arc so that heat is shared between the two plates, usually with a bit more heat on the thicker or lower member, and use a suitable work angle and travel angle.
  • Pause at the sides when weaving. A short dwell at each edge lets the pool fill the toe, then move across quickly through the middle.
  • Use the right electrode or wire diameter and an appropriate wire feed speed for the joint.
  • Use stringer beads or smaller passes if wide weaves cause trouble (see stringer beads vs weaving).
  • Check your gas and your equipment, including whether the gas flow and mix are right for the process.

If undercut shows up only in one position or one joint, change one variable at a time. Test pieces are a cheap way to tune settings.

How undercut is inspected and measured

Undercut is usually found during visual inspection. When it needs to be measured, inspectors use a depth gauge, bridge cam gauge or a similar tool, to measure the depth. Length is measured with a rule. Some codes limit both the depth and the total length of undercut in a given weld length, and depth may be specified in relation to the material thickness. Automated vision systems are also used in production welding to detect undercut.

On pipe, the cap and root are both checked, and undercut on the outside surface is judged separately from internal undercut.

Acceptable limits

There is no universal number. Limits depend on the code and the service of the part. As a general indication only, some structural codes allow shallow undercut on the order of about 1 mm (1/32 in.) for certain statically loaded connections, while limits can be tighter, and sometimes essentially no undercut permitted, for fatigue-loaded or cyclically loaded connections or other critical service. Pipeline, pressure piping and pressure vessel standards each have their own criteria.

Always check the actual edition of the code and the contract specifications that apply. If you are unsure, ask the inspector or engineer who will accept the work.

Repairing undercut

The typical repair depends on the size of the defect and the code:

  1. Clean the area and confirm the extent of the undercut.
  2. Minor undercut can sometimes be blended by light grinding to a smooth profile, if the remaining thickness is acceptable and the code allows it. Grinding must not create a worse notch.
  3. Deeper undercut is normally filled by adding weld metal. Clean the groove, and apply a small stringer bead along the undercut with an appropriate procedure, using a smaller electrode and lower heat so as not to cut a new groove. Preheat may be needed, as it would for the original weld.
  4. Re-inspect the repair, and for crack-prone materials use dye penetrant testing or magnetic particle testing as needed.

Repairs on code work typically need to follow an approved procedure and be documented. If the undercut is a repeated problem, the underlying settings or technique need to be changed rather than repeatedly repairing. For related cracking risks at weld edges and ends, see why welds crack.

The complete guide to weld inspection and defects

Visual Weld Inspection: What to Look For
Read the guide

Keep exploring

Guides from other topics

All topics →