Short answer
Welds crack when the stress on the weld or the surrounding metal is greater than the metal can handle at that moment. The stress usually comes from shrinkage as the weld cools, often made worse by restraint in the joint. Whether the metal can handle it depends on its strength and ductility, which can be reduced by things like hydrogen, brittle microstructure from fast cooling, poor bead shape, contamination, or an unsuitable filler and base metal combination.
To find the actual cause for your weld, you need to look at when and where it cracked.
Work out which type of crack you have
Weld cracks are usually grouped by when they form.
Hot cracks (solidification or liquation cracks) form while the weld is still hot, during or just after solidification.
- Often run along the centerline of the bead, or appear in the crater at the end.
- Linked to shrinkage stress acting on weld metal that is still weak, and to impurities such as sulfur and phosphorus that form low-melting films between grains.
- Are more common with crack-sensitive alloys, deep narrow welds, and highly restrained joints.
Cold cracks (hydrogen-induced or delayed cracks) form after the weld has cooled, sometimes hours or days later.
- Typically start in the heat-affected zone (HAZ) or at the toe of the weld, in hardenable steels.
- Need three things together: hydrogen in the weld, a hard (brittle) microstructure and tensile stress.
Other types include lamellar tearing in thick plate with poor through-thickness properties, and crater cracks (see below).
Cracks that appear right at the end of a bead in a star shape are usually crater cracks, a form of solidification cracking caused by stopping the arc with an unfilled crater.
Common causes
Shrinkage and restraint
Weld metal shrinks as it cools. If the joint is tightly clamped, rigid, or poorly fitted, the shrinkage stress has nowhere to go and the weld can tear. Large root gaps, thick sections and rigid fixtures all raise the stress.
Hydrogen
Moisture, oil, grease, rust, and damp or improperly stored electrodes and flux can introduce hydrogen into the weld pool. Hydrogen can diffuse into the heat-affected zone and, in susceptible steels, contribute to delayed cracking.
Fast cooling and hard microstructures
Thick sections, cold ambient conditions and higher-carbon or alloy steels cool quickly and can form hard, brittle microstructures that are more likely to crack. Preheating and controlling interpass temperature slow cooling and help.
Bead shape
Beads that are very narrow and deep, with a depth-to-width ratio that is too high, tend to be prone to centerline cracking. Concave beads and thin throat sizes in fillet welds are also more prone to cracking, since there is less metal to carry the shrinkage stress.
Crater termination
Breaking the arc abruptly leaves an unfilled, thin crater that cools unevenly and can pull into star-shaped cracks.
Filler and base metal
Using a filler that is not suited to the base metal, or a base metal with high sulfur or phosphorus, can create weld metal that is prone to hot cracking. Dilution of the weld metal by the base metal can also change its composition in unhelpful ways.
Contamination
Dirt, paint, oil, and other contaminants on the joint can add hydrogen or form brittle compounds in the weld.
Cracks in specific materials
- Aluminum: Some aluminum alloys are quite susceptible to solidification cracking. Filler choice matters, and the filler is frequently a different alloy from the base metal. Follow the filler selection guidance from the manufacturer for your specific alloy.
- Carbon and low-alloy steels: Higher carbon content and thicker sections raise hardenability and the risk of hydrogen cracking. Preheat, low-hydrogen consumables and proper storage are the standard defenses.
- Stainless steel: Austenitic grades can be susceptible to hot cracking, and filler composition is chosen with this in mind.
- Cast iron: Very prone to cracking from welding, usually requiring special procedures and preheat.
How to prevent weld cracks
- Clean the joint of rust, oil, paint and moisture.
- Use the right filler metal for the base metal, and store and handle consumables correctly. Keep low-hydrogen electrodes dry.
- Preheat where the material and thickness call for it, and keep the interpass temperature within the limits of the procedure.
- Let the work cool slowly rather than quenching it.
- Fix up the joint well: avoid excessive gaps and unnecessary restraint, and plan the welding sequence to let the parts move.
- Avoid deep, narrow bead profiles. Slower travel speeds and sensible parameters give a more balanced bead.
- Fill the crater before stopping the arc.
- Follow the written procedure. See what WPS, WPQ and PQR mean.
What to do with a cracked weld
Cracks usually need to be removed and the joint rewelded, not just welded over. Grind or gouge out the crack completely, confirm it is gone (for example with penetrant or magnetic particle testing), then reweld using a procedure that addresses the cause, such as with preheat or a different filler. If the part is structural or safety-related, involve a qualified welding engineer or inspector rather than deciding yourself.
Related inspection
Cracks are normally the most serious defect an inspector can find. They are looked for during visual inspection, and fine surface cracks can be revealed by dye penetrant testing. Internal cracks need methods such as ultrasonic testing or radiography.
If you want specific advice for your own weld, note the metal type and thickness, the process, and when and where the crack appeared. Those three details narrow down the cause quickly.