Stick Welding

Stick Welding Amperage Chart: Setting Amps for 6010, 6011, 6013 and 7018

Approximate stick welding amperage ranges for 6010, 6011, 6013 and 7018 by rod size, including 1/8 inch 7018, plus how to adjust for position, thickness and arc behaviour.

On this page
  1. The quick answer for 1/8 inch 7018
  2. Typical amperage ranges
  3. Why ranges differ between brands
  4. Adjusting for position and thickness
  5. Fine-tuning by sight and sound
  6. Machine limits

The quick answer for 1/8 inch 7018

For a 1/8 inch (3.2 mm) E7018 rod, many manufacturers publish a range in the region of about 90 to 150 amps, and a setting around the middle of the range, commonly roughly 110 to 130 amps, is a typical place to start in the flat position. Treat that as a starting point only. The correct range is printed on the rod box or manufacturer data sheet, and it can differ between brands.

Typical amperage ranges

The table below gives approximate ranges that are broadly typical of mild-steel electrodes. They are for orientation, not a procedure. Always check the manufacturer’s recommendation for the specific product.

Rod 3/32 in (2.4 mm) 1/8 in (3.2 mm) 5/32 in (4.0 mm)
E6010 about 40 to 80 A about 75 to 130 A about 90 to 175 A
E6011 about 40 to 80 A about 75 to 130 A about 90 to 175 A
E6013 about 50 to 90 A about 80 to 130 A about 110 to 170 A
E7018 about 70 to 110 A about 90 to 150 A about 120 to 200 A

Rods that need a specific current type are covered in what is AC and DC arc welding, and the character of each rod is in stick welding rods explained.

Why ranges differ between brands

Coating formulations, core wire and manufacturing differ, so one maker’s 1/8 inch 7018 may be rated for a slightly different range than another’s. Rods with higher iron-powder content, for example, are often rated for higher currents. This is why a forum answer of “130 amps” is only a hint.

Adjusting for position and thickness

  • Thin material: use a smaller rod and lower current, otherwise you risk burning through.
  • Thick material: a larger rod and higher current give better fusion, sometimes with multiple passes.
  • Vertical and overhead: generally run at the lower end of the range, or slightly below the flat setting, to keep the puddle small and prevent it from sagging. See overhead welding technique and settings and vertical up welding.
  • Long leads or poor connections: these can reduce the effective current at the arc, so check the clamp (where to put the ground when welding).

For 6013 specifically, many welders run 1/8 inch rods around the lower-to-middle part of the range for overhead work and a little higher in the flat position.

Fine-tuning by sight and sound

Once you are near the published range, adjust by results:

  • Too low: the rod tends to stick, the arc is sluggish, the bead is narrow and ropey and sits on top of the plate. See why your stick electrode keeps sticking.
  • Too high: excessive spatter, a wide, flat, shiny bead, undercut at the edges, a rod that glows red along its length, and a coating that can burn off prematurely.
  • About right: a steady, crisp arc sound (often likened to sizzling bacon), a bead of even width with a good tie-in, and slag that releases cleanly.

Change the current by small steps, such as 5 to 10 amps at a time. The technique of reading the weld is covered in how to lay a weld bead.

Machine limits

Check that your welder can deliver the current you need at its duty cycle, especially with larger rods. A small machine may not run a 5/32 inch rod properly, and running at the top of its output continuously can trip its thermal protection. If it struggles, a smaller rod is usually the answer.

The complete guide to stick welding

How Arc Welding Works: Stick, MMA and the Welding Arc
Read the guide

Keep exploring

Guides from other topics