MIG and TIG Welding

How to TIG aluminum for beginners?

A beginner's guide to TIG welding aluminum: the machine, gas, tungsten and filler you need, cleaning, AC settings, and technique tips for a clean puddle.

On this page
  1. The short answer
  2. Why aluminum is different
  3. What you need
  4. Preparing the aluminum
  5. Machine setup
  6. Technique step by step
  7. Common beginner problems
  8. A simple practice plan

The short answer

To TIG weld aluminum you generally need an AC-capable TIG welder, 100% argon shielding gas, very clean metal and good heat control, usually with a foot pedal. Aluminum conducts heat quickly and is covered by a tough oxide layer that melts at a much higher temperature than the metal underneath, so it behaves differently from steel.

Why aluminum is different

  • The oxide layer. Aluminum forms a thin oxide skin that melts at a far higher temperature than the base metal. Alternating current (AC) helps break it up through a “cleaning action.”
  • Heat conduction. Aluminum pulls heat away quickly, so you often start with high amperage, then ease off as the part heats up. The pedal is useful for this.
  • No color change. Steel glows as it heats; aluminum does not, so you watch for the shiny puddle to form.
  • Contamination. Oil, dirt and moisture cause porosity and a dirty, sooty weld.

What you need

  • An AC/DC TIG welder. DC-only machines cannot weld aluminum properly.
  • 100% argon, typically at roughly 12–20 cubic feet per hour depending on cup size. Follow your machine and cup guidance.
  • A foot pedal for real-time heat control.
  • Tungsten. A 3/32” lanthanated or multi-mix tungsten works for many beginner setups. See choosing TIG tungsten.
  • Filler rod. 4043 is smoother and more forgiving; 5356 is stiffer and stronger. The better choice depends on the base alloy and the application.
  • Cleaning tools. Acetone or alcohol, and a stainless steel brush used only on aluminum.
  • Standard welding PPE, including a welding helmet and gloves.

Preparing the aluminum

  1. Wipe the surface with acetone or alcohol to remove oil and grease.
  2. Brush through the oxide with the dedicated stainless brush, in one direction.
  3. Wipe again, and clean the filler rod too.
  4. Fit the joint tightly. Aluminum fills gaps poorly.
  5. Handle the clean area with clean gloves.

Machine setup

  • Polarity: AC.
  • Amperage: a common starting rule is about one amp per thousandth of an inch of thickness. For 1/8” (0.125”) aluminum, that suggests starting near 125–150 amps and adjusting with the pedal. Thin sheet needs far less.
  • AC balance and frequency: many machines have a default balance that works for beginners. More cleaning action gives a wider etched zone around the weld, while more penetration gives a narrower one. Higher frequency narrows and focuses the arc. Start with defaults and adjust by observing the result.
  • Gas pre-flow and post-flow: use enough post-flow to protect the tungsten and weld while they cool.

Technique step by step

  1. Position the torch with a slight push angle, roughly 5–15 degrees off vertical, with the tungsten close to the work. A short arc, about one tungsten diameter or less, is a good target.
  2. Start the arc and wait for a shiny puddle to form.
  3. Add filler by dabbing it into the leading edge of the puddle, not by melting it in the arc itself.
  4. Keep the filler end inside the gas shield while you move, otherwise it oxidizes.
  5. Move at a steady pace, adjusting the pedal as the part heats up.
  6. At the end, add a touch of filler and ease off the pedal gradually to avoid crater cracks. Some machines can help with this; see 2T and 4T modes if you are using a torch switch instead of a pedal.

Common beginner problems

  • Black, sooty welds: usually contamination or insufficient cleaning, too long an arc, or poor gas coverage.
  • Contaminated tungsten: touching the tungsten to the puddle or the filler. Stop, regrind or reshape it, and restart.
  • Burn-through or sagging: too much heat. Back off the pedal or travel faster, and remember the part keeps heating as you go.
  • Cold, lumpy welds: not enough heat or a puddle that never fully formed.
  • Crater cracks: ending too abruptly.
  • Porosity: dirty metal, a damp filler rod, drafts or a gas leak. Our article on porosity in MIG welds covers many of the same gas-shielding causes.

A simple practice plan

  1. Run beads on a clean 1/8” aluminum plate with no filler to learn puddle control.
  2. Add filler and run straight beads.
  3. Try a T-joint and a lap joint.
  4. Move to thinner and thicker material.

Keep notes on your settings. For how TIG fits among other processes, see MIG and TIG welding.

The complete guide to mig and tig welding

MIG and TIG Welding: How Gas-Shielded Arc Welding Works
Read the guide

Keep exploring

Guides from other topics

All topics →