  1. The short answer
  2. What you need to know before choosing settings
  3. Starting settings for mild steel with C25
  4. How to dial in your settings on scrap
  5. Reading the arc: too low vs too high
  6. Gas flow, stickout and gun angle
  7. Adjustments for CO2, vertical-up and flux-core
  8. Troubleshooting quick table

The short answer

There is no single “good” MIG setting. The right wire feed speed and voltage depend on your material thickness, wire diameter, shielding gas, welding position and the machine itself. The practical approach is to start from a chart, then fine-tune on scrap metal of the same thickness until the arc sounds steady and the bead looks right.

What you need to know before choosing settings

  1. Material and thickness. Thicker metal needs more heat.
  2. Wire type and diameter. Common solid wire sizes for steel are 0.023”, 0.030” and 0.035”.
  3. Shielding gas. Mild steel with a 75% argon / 25% CO2 mix (C25) is the usual reference. See the MIG shielding gas guide.
  4. Position. Flat and horizontal welds tolerate more heat than vertical or overhead.
  5. Machine. Dial markings differ; many machines have a chart inside the wire compartment.

Starting settings for mild steel with C25

These are approximate starting points for flat or horizontal welds with solid wire and C25 gas. Values vary by machine and source, so treat them as a first guess, not a rule.

Steel thickness Wire diameter Voltage (approx.) Wire feed speed (approx.)
22 gauge (about 0.030”) 0.023” 15–17 V 90–110 IPM
18 gauge (about 0.048”) 0.030” 16–18 V 150–170 IPM
16 gauge (about 0.060”) 0.030” 17–20 V 220–250 IPM
1/8” (0.125”) 0.035” 18–22 V 280–320 IPM
3/16” (0.1875”) 0.035” 19–23 V 320–380 IPM
1/4” (0.250”) 0.035” 21–25 V 360–420 IPM

Thicker steel often needs multiple passes or joint preparation, and may exceed the capacity of a small machine. Check your welder’s rated capacity.

How to dial in your settings on scrap

  1. Set the wire feed speed first. It largely determines amperage and heat. See MIG wire feed speed for more.
  2. Set voltage to the chart value.
  3. Run a bead on scrap of the same thickness.
  4. Adjust wire feed speed if the weld looks cold and piled up (increase) or if you risk burn-through (decrease).
  5. Adjust voltage for arc stability and bead shape.
  6. Change one setting at a time and test again.

Reading the arc: too low vs too high

A steady, even sizzle, often compared to bacon frying, is the usual goal in short-circuit transfer.

  • Voltage too low: the wire stubs into the work, you hear a harsh “machine-gun” crackle, and the bead is tall and narrow.
  • Voltage too high: a long arc, a lot of spatter and a flat, wide bead, with a possibility of burn-back to the tip.
  • Wire feed too low: the weld is cold and flat, and the wire may burn back.
  • Wire feed too high: stubbing, pushing the gun back and excess buildup.

Gas flow, stickout and gun angle

  • Gas flow: many guides suggest roughly 15–25 cubic feet per hour for typical shop conditions. Too little leaves the pool exposed, and too much can cause turbulence that pulls air in.
  • Stickout: keep it short and consistent, about 3/8” to 1/2” for smaller wires.
  • Gun angle: about 10–15 degrees off vertical, either pushing or pulling, with a steady travel speed. Moving too fast gives a narrow, weak bead.

Adjustments for CO2, vertical-up and flux-core

  • 100% CO2: often needs slightly higher voltage (roughly 1 V more is a common suggestion) than C25, and it spatters more.
  • Vertical-up: usually uses lower wire feed speed than flat welding to keep the pool under control.
  • Flux-core wire: follow the wire maker’s recommendations. It often runs on different polarity and different settings than solid wire.

Troubleshooting quick table

Problem Likely cause Try
Stubbing, loud crackle Voltage too low or WFS too high Raise voltage slightly or lower WFS
Excess spatter, long arc Voltage too high Lower voltage
Cold, piled-up bead WFS too low Increase WFS
Burn-through Too much heat Lower WFS and voltage, or move faster
Holes in the bead Gas or contamination See porosity in MIG welds

For the bigger picture of how the process works, see MIG and TIG welding.

The complete guide to mig and tig welding

MIG and TIG Welding: How Gas-Shielded Arc Welding Works
Read the guide

Keep exploring

Guides from other topics

All topics →