What porosity is and why it matters
Porosity is small holes or cavities in a weld, caused by gas trapped in the molten pool as it freezes. In MIG welding it usually comes from poor shielding gas coverage or contamination of the metal or wire. Some porosity is merely cosmetic, but on structural or pressure-containing work it can weaken the weld.
Quick diagnosis: what the holes tell you
- Scattered pinholes along the bead: often a gas delivery problem, such as low flow, a leak or a draft.
- Holes that start partway through the weld: the gas may have run out, or something changed such as a gust of wind.
- Larger, deeper holes or “wormholes”: commonly associated with contamination such as oil, rust, paint or moisture.
- Porosity only at the start or end of a bead: check gun position, stickout and gas flow at the arc start.
- Heavy porosity on galvanized or coated steel: the coating vaporizes in the arc.
These are guidelines rather than rules; check multiple possible causes.
Shielding gas problems
- Empty cylinder or closed valve. Check the gauge and that the valve is open.
- Flow too low. The pool is left unprotected. Many shops use roughly 15–25 cubic feet per hour, but check your equipment guidance.
- Flow too high. Turbulence can pull air into the gas stream.
- Leaks. Inspect hoses, fittings, the regulator connection and O-rings. A soapy-water test on connections can show leaks.
- Blocked nozzle or diffuser. Spatter buildup restricts gas flow. Clean or replace the nozzle and check the diffuser holes.
- Faulty solenoid or damaged gun cable. If the gas flows poorly at the gun, the problem may be inside the machine or gun.
See the MIG shielding gas guide for gas choice and flow-rate details.
Drafts and technique
- Wind and fans. Even a light breeze can blow shielding gas away from the arc. Turn off fans, close doors or add a screen.
- Stickout and distance. Holding the gun too far from the work lets air in. Keep stickout short and consistent.
- Steep gun angles. Extreme angles disturb gas coverage. Stay near 10–15 degrees.
- Edges and corners. Welding on outside edges and corners can let gas escape.
- Outdoor welding. Gas-shielded MIG is generally poor in wind; consider self-shielded flux-core wire.
Contamination on the metal
The heat of the arc releases gas from surface contaminants. Common culprits include:
- oil, grease and cutting fluid,
- paint, primer and coatings,
- rust and mill scale,
- moisture and condensation,
- zinc from galvanized steel.
Clean the joint to bright metal on both sides and just beyond the weld zone. Galvanized coatings need special care because zinc fumes are hazardous; remove the coating and ventilate well. See the safety notes in our MIG and TIG overview.
Wire and consumables
- Rusty, oily or moisture-exposed wire can add gas to the pool. Store spools in a dry place.
- A dirty or worn liner can carry contamination into the arc.
- A worn or loose contact tip causes erratic feeding and arc instability.
- A damaged nozzle or missing diffuser leaves the arc unprotected.
Settings and travel speed
Poor parameters can trap gas bubbles. Moving too fast can freeze the pool before gas escapes, and unstable settings can affect gas protection. If everything else checks out, review good MIG settings and wire feed speed.
Step-by-step fix checklist
- Check that there is gas and that the valve is open.
- Verify the flow rate at the gun and check for drafts.
- Inspect hoses, fittings and the regulator for leaks.
- Clean the nozzle and check the diffuser and contact tip.
- Clean the base metal down to bright metal.
- Check the wire for rust or moisture and replace it if needed.
- Lower stickout and correct the gun angle.
- Run a test bead on clean scrap. If it is fine, the problem is the workpiece; if not, it is the equipment or gas.
When porosity matters for the job
For decorative or non-critical work, minor porosity may be acceptable. For structural, pressure, safety-critical or code work, follow the specification or inspection requirements, and grind out and re-weld defective areas as the procedure requires.