Positions and Techniques

What are common TIG welding mistakes?

Common TIG welding mistakes include dirty metal, poor tungsten prep, a long arc, bad gas coverage and filler errors. Learn the causes and how to fix each one.

On this page
  1. The short answer
  2. Preparation mistakes
  3. Setup mistakes
  4. Technique mistakes
  5. Symptom-to-cause table
  6. How to practice to avoid them

The short answer

TIG (GTAW) gives clean, precise welds, but it is unforgiving. The most common mistakes are:

  • Welding on dirty or oxidized metal
  • Contaminating the tungsten or filler rod
  • Poor tungsten preparation or the wrong tungsten for the job
  • Holding too long an arc
  • Wrong polarity, gas flow or shielding setup
  • Pulling the filler rod out of the gas shield
  • Too much heat or moving too slowly
  • Awkward body and hand position that makes steady travel hard

Most of these show up as discolored welds, porosity, an unstable arc or a bead that won’t fuse properly.

Preparation mistakes

Dirty base metal or filler. TIG has little tolerance for contamination. Mill scale, rust, oil, paint and grease cause porosity and a dirty puddle. Clean the joint area with a suitable abrasive or solvent, and handle filler rod with clean gloves. Use a dedicated stainless brush for stainless steel, and keep it away from other metals.

Skipping oxide removal on aluminum. Aluminum has a surface oxide that melts at a much higher temperature than the metal underneath. Remove it just before welding with a stainless brush used only for aluminum or a suitable abrasive, and use AC output so that the arc helps break up the oxide during welding.

Poor tungsten preparation. Common errors are:

  • Grinding the tungsten across the grain instead of lengthwise. Grinding lengthwise, along the electrode, is generally recommended so the arc stays stable.
  • Grinding on a wheel that is also used for other metals, which contaminates the tip.
  • Using a tip shape that doesn’t suit the current. For DC welding, a sharpened point is common; for AC, many welders use a slightly rounded or small balled tip, but follow the guidance for your machine and tungsten type.
  • Breaking a tungsten the wrong way. Scoring it first and then snapping it along the score reduces splits.

Setup mistakes

Wrong polarity. In general, DC electrode negative (DCEN) is used for steel and stainless, and AC is used for aluminum. Check the manual of your machine.

Wrong gas or flow. Pure argon is the usual shielding gas for most TIG work. Too little flow lets air in, and too much creates turbulence that can also draw air into the shield. Check hoses and fittings for leaks and avoid welding in a draft. A flow rate on the order of 15 to 20 cubic feet per hour is a common starting point for argon, but cup size, joint type and environment all matter, so adjust accordingly.

Tungsten stick-out too long. The more tungsten that extends beyond the cup, the less effective the gas coverage. Keep the tungsten as short as the joint allows. Joints with limited access might require a longer stick-out or a gas lens.

No preflow or postflow. Preflow clears air from the torch before the arc starts. Postflow protects the tungsten and the cooling weld. Without postflow, the tungsten often oxidizes and turns blue or black, and the weld edge discolors.

Wrong cup or no gas lens for the joint. A gas lens gives a smoother gas flow and allows a longer tungsten stick-out, which is useful in corners; see welding inside corners and fillet joints.

Technique mistakes

Dipping the tungsten. Touching the tungsten to the puddle or filler contaminates it and the weld. Stop welding, regrind the tungsten, and clean the contaminated spot on the metal before continuing.

Arc too long. A long arc is wide and unfocused. It wanders, reduces gas coverage and gives less penetration. A general rule is to hold the arc length close to the tungsten diameter or a bit more, adjusting for the joint.

Pulling the filler out of the gas shield. The hot end of the rod oxidizes if it leaves the argon. Keep the rod’s tip within the shield when you retract it from the puddle.

Adding filler to the arc instead of the puddle. Dab the filler into the leading edge of the puddle, not into the arc itself. Otherwise it melts off in droplets and doesn’t wet in.

Too much heat, or moving too slowly. Excess heat distorts thin material, and on stainless steel creates heavy discoloration. Establish the puddle quickly, use pulse or lower amperage on thin stock, and keep moving. Using a foot pedal or fingertip control lets you adjust heat mid-weld.

Poor torch and filler angles. A very steep torch angle can disturb the gas and make the puddle hard to see. Typically the torch leans back from the direction of travel by around 10 to 20 degrees, with the filler rod at a low angle to the work. See the discussion of angles in what are the 5 essentials in welding.

Unsupported hands and awkward posture. Without support, the torch wobbles, and the arc length changes. Rest your forearm, wrist or pinky on the work or on a heat-resistant support. Do a dry run of the whole weld path before striking the arc.

Not fitting the joint well. Gaps force you to add more filler and heat. Fit parts tightly, tack them, and check alignment.

Symptom-to-cause table

Symptom Likely causes
Black soot or gray, dirty weld Dirty metal, poor shielding, long arc, filler oxidized
Porosity Contamination, gas leak, wrong flow, draft
Unstable or wandering arc Contaminated or poorly ground tungsten, long arc
Tungsten tip melts or balls up unexpectedly Wrong polarity, too much current for the tungsten size
Rainbow or heavy discoloration on stainless Too much heat, no postflow, poor gas coverage
Burn-through on thin metal Heat too high, travelling too slowly
Lack of fusion Heat too low, filler added too early or too cold

How to practice to avoid them

  • Practice on clean, flat mild steel before trying aluminum or stainless.
  • Run a bead without filler first, to get used to puddle formation and arc length.
  • Add filler once you can hold a steady arc, using a consistent rhythm.
  • Grind several tungstens ahead of time so a dip doesn’t cost you much time.
  • Change one thing at a time when troubleshooting.
  • Review your results by cutting or bending samples to check fusion.

For the positions where TIG gets harder, such as vertical and overhead, see welding positions and techniques for beginners.

The complete guide to positions and techniques

Welding Positions and Techniques for Beginners
Read the guide